Fixing warping and cracking
Many ABS and ASA printing problems come from uneven cooling. Work through these checks in order.
Why it happens
ABS and ASA shrink as they cool. When one part of the print cools faster than another, the plastic pulls on itself. At the bottom, that pull lifts corners off the bed (warping). Higher up, it splits layers apart (cracking or delamination).
Corners lifting off the bed
- Clean the bed. Wash or wipe it according to the bed maker's instructions so there's no oil or dust.
- Check the first layer. It should be slightly squished, not round and loose. Re-level or adjust Z offset if needed.
- Add a brim. A wider brim gives corners more grip.
- Use an adhesion aid suited to your build surface, such as glue stick or a purpose-made adhesive.
- Raise the bed temperature slightly while staying within the limits recommended by your printer and filament manufacturer.
- Turn the first-layer fan off.
Layers cracking or splitting
- Stop drafts. Close the enclosure, or move the printer away from fans, vents, and windows.
- Reduce part cooling. Try the fan fully off for most layers.
- Raise the nozzle temperature in small steps for better layer bonding.
- Preheat the enclosure before you start, and let the print cool in it afterward.
- Slow down a little so each layer has time to bond.
Design changes that help
- Round sharp outside corners with fillets.
- Avoid very long, flat, thin shapes, or split them into parts that join together.
- Add small "mouse ear" discs at corners if a brim isn't enough.
- Orient the part so its largest flat face sits on the bed.
Other things to check
- Wet filament: popping sounds, bubbles, or a rough surface can mean the spool picked up moisture. Dry it following the maker's guidance.
- Bed not heating evenly: large prints may warp only on one side if the bed edges run cooler.
- No enclosure: try a slicer draft shield, or a simple cover around the printer.